top of page
10-1, Loading for Firing
・I leave space at the bottom and top of the kiln, loading the lowest level mainly with taller pieces and the middle levels with shorter items like plates.
・To load the kiln, I place kiln shelves on the shelf supports, set the pieces on the shelves, and stack them one layer at a time. As I go, I ensure the shelves do not interfere with the height of the thermocouples in the lower and upper sections or the color-check hole.
・When handling the pieces, I hold them between the pads of my fingers to prevent the glaze from flaking off, and I carefully place them on the kiln shelves, ensuring they do not stick to one another.
・During the firing process, the upper part inside the kiln heats up quickly and also cools down quickly. Furthermore, the atmosphere varies depending on the location within the kiln, as some areas are more prone to reduction. I consider the type of clay and glaze used in each piece, as well as the desired color and texture tones, to determine the best placement for each piece.
・I load the pieces into the kiln and hope the "kiln god" watches over and excites the flames in the kiln.
10-2, Making test pieces
・I use two methods to assess the condition of my pieces while they’re being fired in the kiln.
・One method involves using Orton cones, specifically No. 8 and 9. Each cone melts at a specific temperature.
・The other method involves using test pieces with three types of glaze. I apply the glazes, usually clear, black, and white, onto small bisque-fired pieces as test pieces. I pull out the pieces with an iron rod toward the end of the firing and check on how the glazes have fired.
・I place the cones and test pieces on a shelf at the same height as the color-check hole on the kiln door.
I visually check on how the two cones have fallen through the color-check hole toward the end of the firing. I pull out one test piece at a time, immediately submerge it in water to cool it, and check on how well the glaze has melted. Since there are three test pieces, I perform this check up to three times.

10-4, Unloading
・I unload the kiln three days after turning off the fire. I don’t want any extreme *kannyu* or cracking on the surface of the pieces, so I open the kiln door gradually to avoid sudden temperature changes. I wait until the temperature inside the kiln has dropped as close as possible to the outside temperature, then open the kiln door a little at first and more a few hours later.
・When the door is completely open, I can hear the "ping, ping" sounds of the glaze cracking.
・I carefully unload the pieces from the kiln.
*Kannyu [Crazing] --- A pattern of fine cracks that appears on glaze surfaces as pieces cool after firing. Cracking occurs because the rates of shrinkage of the ceramic body and the glaze are different.