top of page
Ari's Firing
I use three different firing methods.
For each method, I will fire the kiln for about 20 hours, raising the temperature to about 1246°C.
Firing is performed while restricting the supply of oxygen to the kiln. This causes oxygen to be taken away from the piece.

I add wood immediately after extinguishing the fire during reduction firing. The carbon is absorbed into the clay bodies. (Strong reduction)

Oxidation firing
A method of firing while ensuring a sufficient supply of oxygen.
(h)
(℃)
Ignition – Moisture removal (about 6 hours)
0
6
9
11
14
21
85
500
1200
1240
I open the sliding doors to the studio and turn on the exhaust fan in the kiln room to ensure a smooth airflow and a sufficient supply of oxygen.
I open the kiln damper, open the valve on the oil tank, and ignite the 4 burners. I open the air supply and adjust the oil flow, so that each burner's flame is uniform. I mostly close the kiln door but leave a small gap. After 30 minutes, I check the flames again and make adjustments. *Damper --- A plate located in the exhaust path that is opened or closed to allow or block the flow of gas.
After 3 to 4 hours, I close the door further, leaving a smaller gap.
After another 2 hours, I completely close the door, hold my hand over the 4 viewing holes, and once I can no longer feel any moisture, I close the holes. I attach thermocouples to two locations on the upper and lower parts of the kiln door and set the pyrometer. I set the alarm on the upper thermocouple to 1200°C and turn up the heat.
Firing (about 15 hours)
I increase the heat even more.
(To ensure that the flames of all four burners are uniform, I open the air supply further and adjust the oil flow. I check the color and condition of the flames through the small viewing holes above each burner and the viewing holes at the bottom of the door.)
I increase the heat every two hours. I check the color and condition of the flames through the viewing holes and check the temperature.
Starting around 1200°C, I also pay attention to the temperature difference between the upper and lower areas, and aim to minimize it as much as possible. I try not to adjust the heat too much.
At 1,230°C, I consider the elapsed time and decide the temperature at which to turn off the fire.
I open the color-check hole in the center of the door, ① I visually check the condition of the cones, ② I pull out one test piece, immerse it in water to cool it rapidly, and check how well the glaze has melted.
If the glaze hasn’t melted sufficiently, I set the temperature for turning off the fire slightly higher.
(I open the color-check hole again to check ① and ②.)
If everything looks good, I wait until the firing conditions inside the kiln stabilize, and then hold that temperature for a few minutes longer.
I turn off the fire, close the damper, and close the valve on the oil tank.
Cooling (about 64 hours)
30
To prevent any crazing, I start opening the kiln door once the temperature has dropped to nearly the same as the outside temperature. I open the door gradually over time.


Test pieces removed from the kiln during firing.


The two on the right are test pieces removed during firing.
Reduction firing
A method of firing that restricts the oxygen supply.
(h)
(℃)
Ignition – Moisture removal (about 6 hours)
0
6
9
11
14
21
85
500
1050
1240
I open the sliding doors to the studio and turn on the exhaust fan in the kiln room to ensure a smooth airflow and a sufficient supply of oxygen.
I open the kiln damper, open the valve on the oil tank, and ignite the 4 burners. I open the air supply and adjust the oil flow, so that each burner's flame is uniform. I mostly close the kiln door but leave a small gap. After 30 minutes, I check the flames again and make adjustments. *Damper --- A plate located in the exhaust path that is opened or closed to allow or block the flow of gas.
After 3 to 4 hours, I close the door further, leaving a smaller gap.
After another 2 hours, I completely close the door, hold my hand over the 4 viewing holes, and once I can no longer feel any moisture, I close the holes. I attach thermocouples to two locations on the upper and lower parts of the kiln door and set the pyrometer. I set the alarm on the upper thermocouple to 1050°C (or 950°C, if there are pieces glazed with a copper glaze). And I turn up the heat.
Firing (about 15 hours)
I increase the heat even more.
(To ensure that the flames of all four burners are uniform, I open the air supply further and adjust the oil flow. I check the color and condition of the flames through the small viewing holes above each burner and viewing holes at the bottom of the door.)
I increase the heat every two hours. I check the color and condition of the flames through the viewing holes and check the temperature.
I perform reduction firings at 1,050°C (or 950°C if the pieces are glazed with a copper glaze). I close the damper to an appropriate degree and open the draft. I also narrow the air vent on each burner. This creates an oxygen-deficient environment inside the kiln.
*Draft --- A hole located near the damper in the exhaust passageway to adjust the exhaust force of a chimney. It can also refer to a mechanism that draws in outside air to reduce the exhaust force. Opening this hole reduces the flow of air from inside the kiln to the chimney.
When I open the viewing holes, flames burst out. I periodically check the intensity and condition of the flames and adjust the oil flow accordingly.
At 1100°C, I perform a soot burn off because the firing is taking place in an oxygen-deficient conditions (incomplete combustion) and soot accumulates. I temporarily create an oxidizing state to burn off the soot by opening the damper and closing the draft.
At 1200°C, I again perform a soot burn off.
I pay attention to the temperature differences between the upper and lower areas inside the kiln, and aim to minimize them as much as possible. During reduction firing, the temperatures at the upper and lower areas may reverse. I keep the intensity and condition of the flames consistent while I try not to adjust the heat too much.
At 1,230°C, I consider the elapsed time and decide on the temperature at which to turn off the fire.
I open the color-check hole in the center of the door, ① I visually check the condition of the cones, ② I pull out one test piece, immerse it in water to cool it rapidly, and check how well the glaze has melted.
If the glaze hasn’t melted sufficiently, I set the temperature for turning off the fire slightly higher.
(I open the color-check hole again to check ① and ②.)
If everything looks good, I wait until the firing conditions inside the kiln stabilize, turn off the fire, and close the damper.
I close the draft and the valve on the oil tank.
30
Cooling (about 64 hours)
To prevent any crazing, I start opening the kiln door once the inside temperature has dropped to near outside temperatures. I open the door gradually over time.


I opened draft.


Test pieces removed from the kiln during firing.

Carbonization firing
A method of firing that restricts the oxygen supply, and adds wood at the end of the firing process so the pieces being fired adsorb carbon.

(h)
(℃)
Ignition – Moisture removal (about 6 hours)
0
6
9
11
14
21
85
500
1050
1240
I open the sliding doors to the studio and turn on the exhaust fan in the kiln room to ensure a smooth airflow and a sufficient supply of oxygen.
I open the kiln damper, open the valve on the oil tank, then ignite the 4 burners. I open the air supply and adjust the oil flow, so that the flame on each burner is uniform. I close the kiln door and leave a small gap. After 30 minutes, I check the flames again and make adjustments. *Damper --- A plate located in the exhaust path that is opened or closed to physically allow or block the flow of gas.
After 3 to 4 hours, I close the door further, leaving a small gap.
After another 2 hours, I completely close the door, hold my hand over the 4 viewing holes, and once I can no longer feel any moisture, I close the holes. I attach thermocouples to two locations on the upper and lower parts of the kiln door and set the pyrometer. I set the alarm on the upper thermocouple to 1050°C (or 950°C, if there are pieces glazed with a copper glaze). And I turn up the heat.
Firing (about 15 hours)
I increase the heat even more.
(To ensure that the flames of all four burners are uniform, I open the air supply further and adjust the oil flow. I check the color and condition of the flames through the small viewing holes above each burner and viewing holes at the bottom of the door.)
I increase the heat every two hours. I check the color and condition of the flames through the viewing holes and check the temperature.
I perform reduction firings at 1,050°C (or 950°C if the pieces are glazed with a copper glaze). I close the damper to an appropriate degree and open the draft. I also narrow the air vent on each burner. This creates an oxygen-deficient environment inside the kiln.
*Draft --- A hole located near the damper in the exhaust passageway to adjust the exhaust force of a chimney. It can also refer to a mechanism that draws in outside air to reduce the exhaust force. Opening this hole reduces the flow of air from inside the kiln to the chimney.
When I open the viewing holes, flames burst out. I periodically check the intensity and condition of the flames and adjust the oil flow accordingly.
At 1100°C, I perform a soot burn off because the firing is taking place in an oxygen-deficient conditions (incomplete combustion) and soot accumulates. I temporarily create an oxidizing state to burn off the soot by opening the damper and closing the draft.
At 1200°C, I again perform a soot burn off.
I pay attention to the temperature differences between the upper and lower areas inside the kiln, and aim to minimize them as much as possible. During reduction firing, the temperatures at the upper and lower areas may reverse. I keep the intensity and condition of the flames consistent while I try not to adjust the heat too much.
At 1,230°C, I consider the elapsed time and decide on the temperature at which to turn off the fire.
I open the color-check hole in the center of the door, ① I visually check the condition of the cones, ② I pull out one test piece, immerse it in water to cool it rapidly, and check how well the glaze has melted.
If the glaze hasn’t melted sufficiently, I set the temperature at which I turn off the fire slightly higher.
(I open the color-check hole again to check ① and ②.)
If everything looks good, I wait until the firing conditions inside the kiln stabilize, turn off the fire, and close the damper. I insert shield plates into the burners of all four burners and open the air vents on each burner.
I add wood pieces, as needed. I open the vent at the top of the kiln for a few minutes to increase flame circulation inside the kiln.
I repeat this process two or three times while monitoring conditions until the temperature drops to 1100°C.
I close the draft and close the valve on the oil tank.
Cooling (about 64 hours)
30
To prevent any crazing, I start to open the kiln door once the temperature has dropped to near outside temperatures. I open it gradually over time.
1100

Wood loading port